Fabrication and Evaluation of Organic Field-Effect Transistors (OFETs) : Fullerene C70

Fullerene C70 [F1233]

Fullerene C70 (purified by sublimation)
[for organic electronics]

Fullerene C70
CAS RN: 115383-22-7
Product Number: F1233

Performances of C70 [F1233]-based OFETs

Performances of C70 [F1233]-based OFETs


Table. OFETs Characteristics of Fullerene C70 [F1233]-based OFETs

Entry Fabrication Method Device Configuration SAM Treatment Tsub(°C) Polarity μ (cm2 V−1 s−1) Vth (V) Ion/Ioff
Entry1 Fabrication MethodVacuum deposition Device ConfigurationTCBG SAM TreatmentHMDS Tsub(°C)RT Polarityn μ (cm2 V−1 s−1)0.52 Vth (V)6.7 Ion/Ioff106
Entry2 Fabrication MethodVacuum deposition Device ConfigurationTCBG SAM TreatmentOTS Tsub(°C)RT Polarityn μ (cm2 V−1 s−1)0.55 Vth (V)8.3 Ion/Ioff106

Figure. Transfer curves in the saturated region)

Figure. Transfer curves in the saturated region


Experimental details

Fabrication and evaluation of vacuum-deposited Fullerene C70 [F1233]-based OFETs

< Substrate>
  • HMDS-treated Si/SiO2 (thickness of SiO2: 200 nm)
  • OTS-treated Si/SiO2 (thickness of SiO2: 200 nm)

< Self-Assembly Monolayer (SAM) Treatment>
  • 1,1,1,3,3,3-Hexamethyldisilazane (HMDS) [H0089]
    1. Piranha etching (H2SO4:H2O2=4:1, 80ºC, 2h)
    2. Ultrasonication (Deionized water, Acetone, IPA, 10 min each)
    3. Exposure to vapor (IPA, 3 min)
    4. UV/O3 treatment (1 h)
    5. Immersion in HMDS (16 h, N2)
    6. Ultrasonication (Toluene, Acetone, IPA, 10 min each)
  • n-Octyltrichlorosilane (OTS) [O0168]
    1. Piranha etching (H2SO4:H2O2=4:1, 80ºC, 2h)
    2. Ultrasonication (Deionized water, Acetone, IPA, 10 min each)
    3. Exposure to vapor (IPA, 3 min)
    4. UV/O3 treatment (1 h)
    5. Immersion in OTS solution (0.01 M toluene, 16 h, N2)
    6. Ultrasonication (Toluene, Acetone, IPA, 10 min each)

< Vacuum Deposition>
  • Deposition rate of C70 [F1233] 0.2 Å/s (under a pressure of∼10−5 Pa)
  • Substrate temperature during deposition: RT
  • Deposition rate of Au: 0.2 Å/s (under a pressure of∼10−5 Pa)

< Device configuration>
  • [n+-Si/SiO2 (200 nm) / C70 [F1233] (40 nm) / Au (40 nm)]
  • Top-Contact Bottom-Gate Type (TCBG)
  • Channel Length: 50 μm
  • Channel width: 1.5 mm

< Evaluation condition>
  • Under N2
  • Field-effect mobilities (μ) were determined from the transfer curves in the saturation regime using the following equation:ID = (W/2L) μ Ci (VGVth)2
세션 상태
세션의 남은 시간은 10분입니다. 이대로 방치하면 세션이 끊어지고 탑페이지로 돌아갑니다. 같은 페이지에서 세션을 계속하려면 버튼을 클릭하십시오.분입니다. 이대로 방치하면 세션이 끊어지고 탑페이지로 돌아갑니다. 같은 페이지에서 세션을 계속하려면 버튼을 클릭하십시오.

세션이 시간 초과되었습니다. 탑페이지로 돌아갑니다.