Fabrication and Evaluation of Organic Field-Effect Transistors (OFETs) : trans-DBPen

trans-DBPen [D5488]

Dibenzo[a,l]pentacene
trans-DBPen
CAS RN: 227-09-8
Product Number: D5488

Performance of trans-DBPen [D5488]-based OFETs

Fabrication method and evaluation of vacuum-deposited trans-DBPen [D5488]



Table. OFETs Characteristics of trans-DBPen [D5488]

Entry Fabrication Method Device Configuration SAM Treatment Tsub (°C) Annealing Temp.a (°C) Polarity μ (cm2 V−1 s−1) Vth (V) Ion/Ioff
Entry1 Fabrication MethodVacuum
deposition
Device ConfigurationTCBG SAM Treatmentw/o
Bare
Tsub (°C)60 Annealing Temp.a (°C)120 Polarityp μ (cm2 V−1 s−1)0.16 Vth (V)‒19 Ion/Ioff106
Entry2 Fabrication MethodVacuum
deposition
Device ConfigurationTCBG SAM TreatmentOTS Tsub (°C)60 Annealing Temp.a (°C)120 Polarityp μ (cm2 V−1 s−1)0.44 Vth (V)‒9.8 Ion/Ioff107
Entry3 Fabrication MethodVacuum
deposition
Device ConfigurationTCBG SAM TreatmentODTS Tsub (°C)60 Annealing Temp.a (°C)120 Polarityp μ (cm2 V−1 s−1)0.19 Vth (V)‒6.1 Ion/Ioff106
aPost-annealing temperature.

Figure. Transfer curves in the saturated region

Figure. Transfer curves in the saturated region


Experimental details

Fabrication and evaluation of spin-coated trans-DBPen [D5488]-based OFETs

< Substrate>
  • Bare Si/SiO2 (thickness of SiO2: 200 nm)
  • OTS-treated Si/SiO2 (thickness of SiO2: 200 nm)
  • ODTS-treated Si/SiO2 (thickness of SiO2: 200 nm)

< Self-Assembly Monolayer (SAM) Treatment>
  • n-Octyltrichlorosilane (OTS) [O0168]
    1. Piranha etching (H2SO4:H2O2=4:1, 80ºC, 2h)
    2. Ultrasonication (Deionized water, Acetone, IPA, 10 min each)
    3. Exposure to vapor (IPA, 3 min)
    4. UV/O3 treatment (1 h)
    5. Immersion in OTS solution (0.01 M toluene, 16 h, N2)
    6. Ultrasonication (Toluene, Acetone, IPA, 10 min each)
  • n-Octyltrichlorosilane (ODTS) [T3815]
    1. Piranha etching (H2SO4:H2O2=4:1, 80ºC, 2h)
    2. Ultrasonication (Deionized water, Acetone, IPA, 10 min each)
    3. Exposure to vapor (IPA, 3 min)
    4. UV/O3 treatment (1 h)
    5. Immersion in ODTS solution (0.01 M toluene, 16 h, N2)
    6. Ultrasonication (Toluene, Acetone, IPA, 10 min each)

< Vacuum Deposition>
  • Deposition rate of trans-DBPen [D5488] 0.3 Å/s (under a pressure of∼10−4 Pa)
  • Substrate temperature during deposition: 60 °C
  • Deposition rate of Au: 0.7 Å/s

< Post-Annealing Treatment>
  • Annealing condition: 120 ºC, 5 min, N2

< Device Configuration>
  • [n+-Si/SiO2 (200 nm) / trans-DBPen [D5488] (60 nm) / Au (40 nm)]
  • Top-Contact Bottom-Gate Type (TCBG)
  • Channel Length: 50 μm
  • Channel width: 1.5 mm

< Evaluation Condition>
  • Under N2
  • Field-effect mobilities (μ) were determined from the transfer curves in the saturation regime using the following equation: ID = (W/2L) μ Ci (VGVth)2
Sitzungsstatus
Ihre Sitzung wird in 10 Minuten beendet. Sie werden nach dem Ablauf der Sitzung auf die Startseite umgeleitet. Bitte klicken Sie auf die Schaltfläche, um die Sitzung auf derselben Seite fortzusetzen. Minute beendet. Sie werden nach dem Ablauf der Sitzung auf die Startseite umgeleitet. Bitte klicken Sie auf die Schaltfläche, um die Sitzung auf derselben Seite fortzusetzen.